Gas Permeability after Gelbo Flex Text
| Text Condition : |
 |
Gelbo Flex Tester (product of Tester Industries corp.) |
|
Stroke : 40 cycle/min, Twisting : 440 , Horizontal movement : 2.5 inch |
|
Atmosphere 23 , 50%RH |
| Gas Barrier Material |
Layer Structure |
O2TR 25 , 80%RH cc/m2 d atm |
WVTR 40 , 90%RH g/m2 d |
| None |
After 10 times Gelbo Flex |
None |
After 10 times Gelbo Flex |
TECHBARRIER -V |
V(SiOx) / LL50 |
0.7 |
10 |
0.7 |
1 |
TECHBARRIER -P2 |
P2(SiOx) / LL50 |
0.5 |
10 |
0.3 |
1 |
TECHBARRIER -H |
H(SiOx) / LL50 |
0.3 |
10 |
0.3 |
1 |
TECHBARRIER -T |
PET12 / (SiOx)T / CPP50 |
0.3 |
10 |
0.3 |
1 |
TECHBARRIER -NY |
NY(SiOx)T / LL50 |
0.5 |
10 |
0.7 |
2 |
TECHBARRIER -NR |
PET12 / (SiOx)NR / CPP50 |
0.5 |
10 |
0.7 |
2 |
TECHBARRIER -S |
OPP20 / (SiOX)S / CPP50 |
< 0.1 |
0.3 |
0.1 |
0.3 |
|
| AL-Metallized OPET |
AL-Metallized OPET12(Met) / LL50 |
1.2 |
10 |
0.5 |
3 |
| AL foil |
OPET12 / AL9 / CPP50 |
< 0.1 |
20 |
0.1 |
0.2 |
The above data is just a test result, but not guaranteed.
|