Mitsubishi Plastics, Inc.
TECHBARRIER
Table 1. Retort / Boiling Durability

Gas Transmission Rate after Retort / Boiling

TECHBARRIER-NR, T, TZ
  TECHBARRIER NR T TZ
Retort / Boiling Condition OPET12//NR//
CPP50
OPET12//T//
CPP50
TZ//OPA15//
CPP50
O2TR
cc/m2datm

25, 80%RH
None 0.5 0.3 1.0
80, 30 min - - -
90, 30 min - - -
100, 30 min - - -
110, 30 min 0.5 0.5 -
120, 30 min 0.7 0.5 1.3
130, 30 min      
WVTR
g/m2d

40, 90%RH
None 0.7 0.3 0.7
90, 30 min - - -
120, 30 min 1.0 0.5 0.7
130, 30 min      
Base Film ONY OPET

TECHBARRIER-L, H, V
  TECHBARRIER L H V
Retort / Boiling Condition L//CPP50 L//LL50 H//LL50 V//LL50
O2TR
cc/m2datm

25, 80%RH
None 0.5 0.5 0.3 0.7
80, 30 min     0.5 1.0
90, 30 min   1.0 0.5 2.0
100, 30 min   1.0 2.5 4.0
110, 30 min 1.0   - -
120, 30 min 1.0   - -
130, 30 min 2.5      
WVTR
g/m2d

40, 90%RH
None 0.3 0.3 0.3 0.7
90, 30 min 0.5 0.5 0.5 1.5
120, 30 min 0.5 - - -
130, 30 min 1.0 -    
Base Film OPET

The above data is just a result of our test, but not guaranteed.



Copyright 2002 by Mitsubishi Plastics,Inc. All Rights Reserved.
BACK

Back to HOME